_files/10px.gif) |
Nylon
Technical Data
Nylon
Type 6/6
_files/10px.gif)
| PROPERTIES |
UNITS |
ASTM METHOD |
0.2% WATER |
2.5% |
_files/str.gif) _files/10px.gif) |
Tensile
Strength |
-40°F 73°F 170°F |
psi psi psi
_files/10px.gif) |
0-638 D-638 0-638 |
— 12,600 8,500 |
16,100 11,200 5,900 |
| Yield
Stress |
-40°F 73°F 170°F |
psi psi psi
_files/10px.gif) |
D-638 D-638 D-638 |
— 12,600 8,500 |
16,100 8,600 — |
| Elongation
at Break |
-40°F 73°F 170°F |
|
D-638 0-638 D-638
_files/10px.gif) |
— 90 155 |
35 300 350 |
| Shear Strength |
psi
_files/10px.gif) |
0-732 |
9,600 |
— |
_files/sti.gif) _files/10px.gif) |
Flexural
Modulus |
-40°F 73°F 170°F |
psi psi psi
_files/10px.gif) |
D-790 0-790 0-790 |
470,000 410,000 100,000 |
500,000 175,000 — |
Compressive Stress at 1% Def Deformation under Load
(2000 psi,122°F) Deflection Temp.,
_files/10px.gif)
|
66
psi 264psi
_files/10px.gif) |
psi % °F °F |
D-695 D-621 D-648 D-648 |
4,900 1.4 470 220 |
— — — — |
_files/10px.gif)
_files/tou.gif)
_files/10px.gif) |
Brittleness Temp. Izod Impact Strength |
-40°F 73°F |
°F ft.lb/in. ft.lb/in. |
D-746 D-256 D-256 |
-148 — 1.3 |
-121 — 2.5 |
_files/10px.gif)
_files/the.gif)
_files/10px.gif) |
Melting Point (Fisher-Johns) Melting Point
(Crystalline) Coefficient of Linear Thermal Expan.
_files/10px.gif) |
°F °F in./in./°F |
D-789
D-696 |
482-500 518 — |
— — — |
Specific Heat Thermal Conductivity
_files/10px.gif) |
B.T.U./hr./ sq.ft./°F/in. |
(5) |
0.3-0.5
1.7 |
—
— |
_files/ele.gif) |
Volume
Resistivity Dielectric Contant, |
100Hz(cps) 10to3rdHz(cps) 10to6thHz(cps)
_files/10px.gif) |
ohm-cm |
D-257 D-150 D-150 D-150 |
10 to
15th 4.0 3.9 3.6 |
10 to
13th 6.0 5.1 4.1 |
| Power
Factor |
100Hz(cps) 10to3rdHz(cps) 10to6thHz(cps)
_files/10px.gif) |
|
D-150 D-150 D-150 |
0.03 0.03 0.04 |
0.04 0.04 0.05 |
_files/mis.gif) |
Specified Gravity Hardness, Rockwell
_files/10px.gif) |
|
D-792 D-785 |
1.13-1.15 R118,M79 |
— R108,M59 |
Water Absorption (24 hr.) Water absorption
(Saturation)
_files/10px.gif) |
% % |
D-570 D-570 |
1.5 8.5 |
— — |
Taber Abrasion, CS-17 Wheel, 1000g Flammability
(Class)
_files/10px.gif) |
mg./1000
Cycles |
UL-95(9) |
— — |
3.5 94V-2 |
Nylon •
Ohmoid Phenolics
• Fibre •
Delrin
|